PRODUCTS

eSPAÑOLEnglish

INSULATING BRICKS


Fireclay Insulating Brick(B)
 
Properties
 
INDEX
ITEMS
NG-1.5
NG-1.3a
NG-1.3b
NG-1.0
NG-0.9
NG-0.8
NG-0.7
NG-0.6
NG-0.5
NG-0.4
Volume Density, g/cm 3
1.5
1.3
1.3
1.0
0.9
0.8
0.7
0.6
0.5
0.4
C.C.Strength, MPa
55
40
350
25
20
20
15
10
10
8
the Linear Change after Reheating Not More than 2%,the Test Temperature, ℃
1300
1300
1250
1250
1200
1150
1150
1100
1050
1050
the Thermal Conductivity W/m · k , Average Temperature 350 ± 25 ℃ , =
0.7
0.60
0.60
0.50
0.40
0.35
0.35
0.25
0.25
0.2